A cable designer once told us their TPEE jacket was rated to 218 °C because that was the melting point. The UL card said 85 °C. Melting point, RTI, heat deflection temperature and brittleness temperature answer four different questions — mixing them is the most common specification error in this material. For EV charging, the numbers that matter are the RTI, the halogen-free flame-retardant construction, and the water temperature rating.
The four numbers buyers confuse
Number | What it actually answers | Typical misunderstanding |
Melting point, ISO 11357 | Crystal phase change | Treated as the continuous service limit |
UL 746B RTI | Long-term thermal ceiling, per property and thickness | Ignored, or quoted as a single figure |
HDT at 1.8 MPa | Temperature at which a loaded specimen deflects | Confused with load-bearing service temperature |
Brittleness, ISO 974 | Standard embrittlement test result | Applied directly to a finished cable construction |
A jacket running at 90 °C needs a grade and a construction whose RTI supports it — not a grade with a high melting point. Where a supplier quotes 120–150 °C without a UL card behind it, ask what test produced that number.
Halogen-free flame retardancy: not all FR grades are equal
For charging cables and harness protection, the flame-retardant system matters as much as the base resin. Halogen-free V-0 systems exist in TPEE, but some concentrates are brominated and therefore not halogen-free. Ask for the specific grade designation and the combustion test report, not a generic "flame retardant TPEE" label.
A second concern is additive bloom. In high-voltage insulation, a migrating flame-retardant additive can attack copper conductors and contacts. Specify a compound with controlled additive mobility and verify it against your insulation stack.
The 90 °C water table
Hot water is the environmental limit that catches TPEE buyers out. Ester hydrolysis scissions the chain and the released acid autocatalyses further scission; the rate roughly doubles for every 10 °C rise. Harder grades, despite their higher modulus, are often rated "not recommended" at 90 °C while softer grades remain "possibly resistant."
Requirement | Recommended route | What to verify |
Outdoor jacket, ambient moisture | Light-stabilised TPEE | UV package and colour stability |
90 °C water exposure | Hydrolysis-stabilised, softer grade | Water rating at the actual temperature |
Halogen-free V-0 | Halogen-free FR compound | UL94 report and CTI value |
Flex at low temperature | Low-temperature toughened grade | Bend test on the finished construction |
High-voltage insulation | Controlled-bloom FR compound | Copper compatibility data |
Extrusion details that change the outcome
A TPEE jacket runs through a cross-head. Die selection decides whether the melt meets the core under pressure or as a drawn-down tube:
Die type | How melt meets the core | Best for |
Pressure / packing die | In-die, under pressure | Adhesion to a rough core |
Tubing / sleeving die | Drawn down, often with vacuum | Wall control and clean stripping |
Melt temperature must be measured at the die, not inferred from barrel settings. TPEE viscosity can change several-fold over a small temperature interval, and a jacket that looks fine at startup can drift out of tolerance as the barrel warms. Dry the resin to the grade's moisture ceiling before extrusion — hydrolysis in the barrel will not show up until the cable is in service.

Extrusion details change the outcome
What we supply from Changzhou
At DOWREN's own facility in Changzhou, we compound cable grades against the construction rather than the datasheet. A typical EV charging enquiry arrives with four requirements — a temperature ceiling, a flame-retardant standard, a water exposure condition and a bend radius — and no single catalogue grade that satisfies all four.
Our approach is to select the base resin for the dominant demand, then adjust the package: a halogen-free FR system with controlled bloom, a hydrolysis stabiliser where water is present, and a light-stable colour system for outdoor use. We have produced 55D halogen-free V-0 grades for harness protection and hydrolysis-stabilised softer grades for wet service, each with a defined test protocol.
Verification and documents
For cable projects we provide the grade-specific TDS, the UL or EN construction reference where applicable, a lot-level COA, RoHS and REACH declarations, and the flame-retardant test report. Where the customer requires a specific cable standard, we confirm the exact construction before sampling. Trial quantities of 1 kg, 5 kg and 10 kg are packed in moisture-barrier film and shipped from Changzhou.
Send us the construction
Tell us the conductor size, the jacket thickness, the required temperature rating, the flame standard and the water exposure. Our application team will shortlist a grade or propose a modified compound, and arrange an extrusion trial with samples.
DOWREN NEW MATERIAL (HENAN) CO.,LTD
TELL:Selina.Liu +86-0393-8993626 / +86 18137458807
ADD:150 meters north of the intersection of Zhongyuan Road and Pushang Road, Puyang City,Henan Province
EMAIL:dowren@dowren.com
WhatsApp (+86 18137458807)