TPEE Hydrolysis: Why Standard Grades Fail in Hot Water
Time of issue:2026-11-09 09:00
source:
author:

TPEE hydrolysis is not gradual ageing. Water attacks the ester links in the polyester hard segment and releases carboxylic acid; that acid then catalyses further scission. Once the reaction passes its threshold it accelerates. The practical answer is a two-line defence: control moisture before processing, and specify a hydrolysis-stabilised compound whose additive package consumes the acid as it forms.
The failure that looks like a material defect
A maker of industrial tubing came to us with parts that had become white, brittle and weak after several months in warm water service. The resin was a high-hardness general-purpose TPEE — chosen because the buyer believed "harder means better." The parts passed the initial tensile test and failed in the field.
This pattern is common enough that we keep a water-resistance table in our technical files, because the grade choice surprises people every time.
The chemistry, in plain terms
The polyester hard segment contains ester bonds. In hot water, those bonds cleave and produce carboxyl end groups. The carboxylic acid released by the first cleavage catalyses the next one, so the rate increases as degradation proceeds — a self-accelerating loop. The visible signs follow: surface whitening, embrittlement, and a steep drop in tensile strength rather than a gentle decline.
Two engineering consequences follow directly. First, a short damp-heat test can look acceptable while long-term service fails, because the test may end before the catalytic loop takes hold. Second, adding a hydrolysis stabiliser at too low a dose does not help: the protection is stoichiometric, not physical. The additive must cover the acid equivalents that will be generated.
The 90 °C water table buyers misread
Grade family | Hardness | Water at 23 °C | Deionised water at 90 °C |
Softer general-purpose grades | 40D–55D | Possibly resistant | Possibly resistant |
Harder high-modulus grades | 63D–82D | Possibly resistant | Not recommended |
FR concentrate on a 55D base | 55D | Possibly resistant | Not recommended |
The counter-intuitive lesson: the harder grade with the higher modulus is often *worse* in hot water, because its higher hard-segment content gives the reaction more ester bonds to attack. Hardness is not a proxy for hydrothermal stability.
This matters for electric-vehicle charging jackets and battery cooling loops, where a 90 °C water rating may be part of the specification. The grade that looks strongest on the datasheet can be the wrong one in the water table.

The 90 °C water table buyers misread
Moisture control comes before any additive
A carbodiimide package deals with acid that has already formed and water already in the system. It cannot undo chain scission that happened in the barrel before the additive had a chance to act. In our Changzhou plant, we treat drying as a hard gate: dehumidifying dryer, 100–120 °C for 3–4 hours, and a verified moisture ceiling before the run. For the most sensitive grades we use a dehumidifying dryer with a monitored dew point rather than a hot-air oven.
Regrind deserves the same discipline. Each pass shortens chains, and regrind that has absorbed humidity can reintroduce water even when virgin pellets were dry.
What we compound instead
At DOWREN's own facility in Changzhou, hydrolysis resistance is a designed property, not a catalogue option. The variables we adjust are:
Compound variable | What we change | Why |
Base resin | Polyether soft-segment grade where oil resistance permits | Fewer hydrolysable links in the soft phase |
Stabiliser package | Polymeric carbodiimide in the functional window | Consumes carboxylic acid as it forms |
Co-stabiliser | Selected antioxidant / co-stabiliser for severe service | Extends protection beyond a single component |
End-group control | Grade with reduced reactive end groups | Removes the initiation site |
Colour package | Non-acidic pigment and carrier system | Avoids introducing catalytic residues |
The aim is not to pass a short damp-heat screen. It is to keep mechanical properties stable over the intended service life, under the actual temperature and pH of the application.

A stabilised compound changes the outcome
Verification and documents
For hydrolysis-critical projects we agree the test protocol before sampling: 85 °C / 85% RH exposure, hot-water immersion at the service temperature, or a customer-specificcycle. We report tensile and elongation retention at defined intervals, not a single pass/fail point. Every lot ships with a lot-level COA, and we supply the TDS plus RoHS and REACH declarations with the sample pack.
Send us the service conditions
Tell us the water or humidity temperature, the exposure duration, the pH or fluid chemistry, and whether the part is under load. Our Changzhou application team will propose a standard hydrolysis-resistant grade or a custom stabilised compound, and provide 1 kg, 5 kg or 10 kg moisture-barrier samples for validation.
DOWREN NEW MATERIAL (HENAN) CO.,LTD
TELL:Selina.Liu +86-0393-8993626 / +86 18137458807
ADD:150 meters north of the intersection of Zhongyuan Road and Pushang Road, Puyang City,Henan Province
EMAIL:dowren@dowren.com
WhatsApp (+86 18137458807)